USA UNS S44700
Corresponding Standard ASTM A580/A580M-2018
Stainless Steel Wire
Classification Ferritic Stainless Steel
Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N More
Minimum Value - - - - - 28 - - 3.5 - C+N 0.025
Maximum Value 0.01 0.2 0.3 0.025 0.02 30 0.15 0.15 4.2 0.02
Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
A Cold Precision Rolling ≥520 ≥415 ≥15 ≥30
A Annealing ≥485 ≥380 ≥20 ≥40
Approximate Comparison Table Ferritic Stainless Steel
China Japan United States International Organization for Standardization European Standard
ISC JIS UNS ISO Numerical Grade Numerical Grade
S13091 SUS447J1 S44700 X1CrMo30-2 4135-447-92-C (1.4135)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!