Grade C30
Corresponding Standard ISO 683-1-2016
Non-alloy steels for quenching and tempering
Classification Carbon Steel
C30 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.27 0.1 0.5 - - - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.34 0.4 0.8 0.045 0.045 0.4 0.4 0.3 0.1
C30 Mechanical Properties
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
d≤16 or t≤8 600~750 ≥400 ≥18
16<d≤40 or 8<t≤20 550~700 ≥350 ≥20
Round products d≤63, flat products d≤35 500~650 ≥300 ≥21
1 Approximate Comparison Table Carbon Structural Steel and Engineering Steel
China Japan International Organization for Standardization
GB JIS ISO
30 S30C C30
2 Approximate Comparison Table High-Quality Carbon Structural Steel
China Japan United States International Organization for Standardization Germany France European Standard Russia United Kingdom
GB JIS SAE ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade GOST BS EN/BS
30 S30C 1030 C30
C30E4
C30
Ck30
1.0528 AF50C30
XC32
C30 1.0528 30 080M32
En5
3 Approximate Comparison Table High-Quality Carbon Structural Steel
China Japan United States International Organization for Standardization France Russia United Kingdom
GB JIS ASTM/AISI ISO NF EN/NF GOST BS EN/BS
GB/T 699-1999
30
S30C 1030 ISO 630-1:1987
C30
C30E4
C30M2
C30
XC32
30 060A30