Grade C25R
Corresponding Standard ISO 683-1-2016
Non-Alloy Steels for Quenching and Tempering
Classification Carbon Steel
C25R Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.22 0.1 0.4 - 0.02 - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.29 0.4 0.7 0.025 0.04 0.4 0.4 0.3 0.1
C25R Mechanical Properties
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
d≤16 or t≤8 550~700 ≥370 ≥19 ≥35
16<d≤40 or 8<t≤20 500~650 ≥320 ≥21 ≥35
Approximate Comparison Table Non-Alloy Steel for Quenching and Tempering
International Organization for Standardization Germany France European Standard
ISO DIN EN/DIN NF EN/NF EN Numerical Grade
C25R Cm22 XC18u C22R
C22R
1.1149
C25R Corresponding Standards(Same grade name, different standards)