Grade C40R
Corresponding Standard ISO 683-1-2016
Non-alloy steels for quenching and tempering
Classification Carbon Steel
C40R Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.37 0.1 0.5 - 0.02 - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.44 0.4 0.8 0.025 0.04 0.4 0.4 0.3 0.1
C40R Mechanical Properties
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Impact Energy Absorption
KV2
J
d≤16 or t≤8 650~800 ≥460 ≥16 ≥35 ≥20
16<d≤40 or 8<t≤20 630~780 ≥400 ≥18 ≥40 ≥20
40<d≤100 or 20<t≤60 600~750 ≥350 ≥19 ≥45 ≥20
Approximate Comparison Table Non-Alloy Steel for Quenching and Tempering
United States International Organization for Standardization Germany France European Standard
ASTM ISO DIN EN/DIN NF EN/NF EN Numerical Grade
1040 C40R
C40M2
Cm40 XC42H1u C40R 1.1189
C40R Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!