Grade C60R
Corresponding Standard ISO 683-1-2016
Non-alloy steels for quenching and tempering
Classification Carbon Steel
C60R Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.57 0.1 0.6 - 0.02 - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.65 0.4 0.9 0.025 0.04 0.4 0.4 0.3 0.1
C60R Mechanical Properties
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
d≤16 or t≤8 850~1000 ≥580 ≥11 ≥25
16<d≤40 or 8<t≤20 800~950 ≥520 ≥13 ≥30
40<d≤100 or 20<t≤60 750~900 ≥450 ≥14 ≥35
Approximate Comparison Table Non-Alloy Steel for Quenching and Tempering
International Organization for Standardization Germany European Standard
ISO DIN EN/DIN EN Numerical Grade
C60R
C60M2
Cm60 C60R 1.1223
C60R Corresponding Standards(Same grade name, different standards)