Grade 13CrMo 4-5
Corresponding Standard ISO 9330-4-2000
Submerged arc-welded unalloyed and alloyed steel tubes with specified elevated temperature properties
Classification Alloy Steel
13CrMo 4-5 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Cu Mo Al
Minimum Value 0.1 0.15 0.4 - - 0.7 - 0.4 -
Maximum Value 0.17 0.35 0.7 0.035 0.03 1.1 0.25 0.6 0.02
13CrMo 4-5 Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤40 Normalizing 900~960°C, tempering 660~730°C, air cooling 440~590 ≥290 Longitudinal, ≥ 22; Transverse, ≥ 20 t > 30, Transverse
27
40<t≤60 Normalizing 900~960°C, tempering 660~730°C, air cooling 440~590 ≥280 Longitudinal, ≥ 22; Transverse, ≥ 20 Transverse
27
Approximate Comparison Table
China United States International Organization for Standardization European Standard Russia
GB ASTM ISO EN Numerical Grade GOST
15CrMoR
GB/T 713.2-2023
SA387 Gr.12
ASME Ⅱ-A-2021
13CrMo4-5
ISO 9328-2018
13CrMo4-5
EN 10028-2017
1.7335 12ХМ

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!