Grade 23MnB4
Germany W-Nr. 1.5535
Corresponding Standard DIN EN 10263-4-2018
Steel rod, bars and wire for cold heading and cold extrusion Part 4: Technical delivery conditions for steels for quenching and tempering
Classification Alloy Steel
23MnB4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Cu B
Minimum Value 0.2 - 0.9 - - - - 0.0008
Maximum Value 0.25 0.3 1.2 0.025 0.025 0.3 0.25 0.005
23MnB4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Reduction of Area
ψ
%
Bar, rod, wire; 5<d≤25 Untreated or Pickling (+U or +PE) ≤600 ≥60
Bar, rod, wire; 5<d≤25 Spheroidizing or Spheroidizing and Peeling (+AC or +AC+PE) ≤520 ≥64
Wire; 5<d≤10 Untreated and Cold Drawn (+U+C) ≤700 ≥55
Wires; 10<d≤25 Untreated and Cold Drawn (+U+C) ≤690 ≥55
Wire; 2<d≤5 Unheated, Cold Drawn, and Spheroidized (+U+C+AC) ≤510 ≥66
Wire Rods; 5<d≤25 Unheated, Cold Drawn, and Spheroidized (+U+C+AC) ≤500 ≥66
Wire; 2<d≤5 Unheated, Cold Drawn, Spheroidized, and Quenched Rolling (+U+C+AC+LC) ≤550 ≥64
Wire Rods; 5<d≤25 Unheated, Cold Drawn, Spheroidized, and Quenched Rolling (+U+C+AC+LC) ≤540 ≥64
Wire; 5<d≤10 Spheroidizing + Cold Drawn (+AC+C) ≤620 ≥59
Wires; 10<d≤25 Spheroidizing + Cold Drawn (+AC+C) ≤610 ≥59

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!