Grade
37MnB5
Germany W-Nr.
1.5538
Corresponding Standard
DIN EN 10263-4-2018
Steel rod, bars and wire for cold heading and cold extrusion Part 4: Technical delivery conditions for steels for quenching and tempering
Classification
Alloy Steel
37MnB5 Chemical Element Composition Content (%)
Component
C
Si ⓔ
Mn
P
S
Cr ⓕ
Cu
B
Minimum Value
0.35
-
1.15
-
-
-
-
0.0008
Maximum Value
0.4
0.3
1.45
0.025
0.025
0.3
0.25
0.005
37MnB5 Mechanical Properties
condition
Heat Treatment or Condition
Tensile Strength σb
Mpa
Reduction of Area ψ
%
Bars, rods, wires; 5<d≤40
Spheroidizing or Spheroidizing and Peeling (+AC or +AC+PE)
≤620
≥62
Wire; 2<d≤5
Unheated, Cold Drawn, and Spheroidized (+U+C+AC)
≤610
≥64
Wire; 5<d≤40
Unheated, Cold Drawn, and Spheroidized (+U+C+AC)
≤600
≥64
Wire; 2<d≤5
Unheated, Cold Drawn, Spheroidized, and Quenched Rolling (+U+C+AC+LC)
≤650
≥62
Wire; 5<d≤40
Unheated, Cold Drawn, Spheroidized, and Quenched Rolling (+U+C+AC+LC)
≤640
≥62
Wire; 5<d≤40
Spheroidizing + Cold Drawn (+AC+C)
≤720
≥57
37MnB5 Corresponding Standards(Same grade name, different standards)