Grade
37Mo2
European Standard Steel Grade
1.5418
Corresponding Standard
EN 10263-4-2017
Steel Rod, Bars and Wire For Cold Heading and Cold Extrusion Part 4: Technical Delivery Conditions for Steels for Quenching and Tempering
Classification
Alloy Steel
37Mo2 Chemical Element Composition Content (%)
Component
C ⓓ
Si ⓔ
Mn
P
S
Cu
Mo
Minimum Value
0.35
-
0.6
-
-
-
0.2
Maximum Value
0.4
0.3
0.9
0.025
0.025
0.25
0.3
37Mo2 Mechanical Properties
condition
Heat Treatment or Condition
Tensile Strength σb
ksi
Hardness
HBW
Wire; 2<d≤5
Spheroidizing + Cold Drawn + Spheroidizing (+AC+C+AC)
≤560
≥61
Wire; 5<d≤40
Spheroidizing + Cold Drawn + Spheroidizing (+AC+C+AC)
≤550
≥61
Bars, wires; 2<d≤5
Spheroidizing + Cold Drawn + Spheroidizing + Quenched Rolling (+AC+C+AC+LC)
≤600
≥59
Bars, wires; 5<d≤40
Spheroidizing + Cold Drawn + Spheroidizing + Quenched Rolling (+AC+C+AC+LC)
≤590
≥59
Bars, rods, wires; 5<d≤40
Spheroidizing or Spheroidizing + Rotary Peeling (+AC or +AC+PE)
≤570
≥59
Approximate Comparison Table Steel for Cold Heading and Cold Extrusion
International Organization for Standardization
European Standard
ISO
EN
Numerical Grade
37Mo2
37Mo2
1.5418
37Mo2 Corresponding Standards(Same grade name, different standards)