Grade 28CrS4
Germany W-Nr. 1.7036
Corresponding Standard DIN 17200-1987
Classification Alloy Steel
28CrS4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr
Minimum Value 0.24 - 0.6 - 0.02 0.9
Maximum Value 0.31 0.4 0.9 0.035 0.035 1.2
28CrS4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
All Sizes Shearable condition (C) ≤255
All Sizes Softening Annealing (G) ≤217
d≤16 Quenching and Tempering (V) 850~1000 ≥650 ≥12 ≥40 ISO-V
≥35
16<d≤40 Quenching and Tempering (V) 750~900 ≥550 ≥14 ≥45 ≥40
40<d≤100 Quenching and Tempering (V) 650~800 ≥410 ≥15 ≥50 ≥45
Approximate Comparison Table structural alloy steel
International Organization for Standardization Germany European Standard
ISO DIN EN/DIN EN Numerical Grade
28CrS4 28CrS4 28CrS4 1.7036

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!