Grade 30CrMoV9
Germany W-Nr. 1.7707
Corresponding Standard DIN 17200-1987
Steels for Quenching and Tempering; Technical Delivery Conditions
Classification Alloy Steel
Properties High Strength
30CrMoV9 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Mo V
Minimum Value 0.26 - 0.4 - - 2.3 0.15 0.1
Maximum Value 0.34 0.4 0.7 0.035 0.03 2.7 0.25 0.2
30CrMoV9 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Steel; All Sizes Softening Annealing (G) ≤248
Steel; d≤16 Quenching and Tempering (V) 1250~1450 ≥1050 ≥9 ≥35 ISO-V
≥25
Steel; 16<d≤40 Quenching and Tempering (V) 1200~1450 ≥1020 ≥9 ≥35 ≥25
Steel; 40<d≤100 Quenching and Tempering (V) 1100~1300 ≥900 ≥10 ≥40 ≥30
Steel; 100<d≤160 Quenching and Tempering (V) 1000~1200 ≥800 ≥11 ≥45 ≥35
Steel; 160<d≤250 Quenching and Tempering (V) 900~1100 ≥700 ≥12 ≥50 ≥45
Approximate Comparison Table Structural Alloy Steel
China Germany European Standard
GB DIN EN/DIN W-Nr. EN Numerical Grade
30Cr2MoV 30CrMoV9 1.7707 30CrMoV9 1.7707
30CrMoV9 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!