Grade C25R
Corresponding Standard DIN EN ISO 683-1-2018
Heat-Treatable Steels,alloy Steels and Free-Cutting Steels--Part 1: Non-Alloy Steels for Quenching and Tempering
Classification Carbon Steel
C25R Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.22 0.1 0.4 - 0.02 - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.29 0.4 0.7 0.025 0.04 0.4 0.4 0.3 0.1
C25R Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
d≤16; t≤8 Quenching and Tempering 550~700 ≥370 ≥19 ≥35
16<d≤40;8<t≤20 Quenching and Tempering 500~650 ≥320 ≥21 ≥35
d≤16;t≤16 Normalizing (N) ≥470 ≥260 ≥22
16<d≤100;16<t≤100 Normalizing (N) ≥440 ≥230 ≥23
New and Old Grade Replacement List
Corresponding Standard Grade
DIN 17200-1987
Grade
Germany W-Nr.
DIN EN ISO 683-1-2018
Grade
C25R Corresponding Standards(Same grade name, different standards)