Grade C40R
Corresponding Standard DIN EN ISO 683-1-2018
Heat-treatable steels,alloy steels and free-cutting steels--Part 1: Non-alloy steels for quenching and tempering
Classification Carbon Steel
C40R Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.37 0.1 0.5 - 0.02 - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.44 0.4 0.8 0.025 0.04 0.4 0.4 0.3 0.1
C40R Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Impact Energy Absorption
KV2
J
d≤16; t≤8 Quenching and Tempering 650~800 ≥460 ≥16 ≥35 ≥20
16<d≤40;8<t≤20 Quenching and Tempering 630~780 ≥400 ≥18 ≥40 ≥20
40<d≤100;20<t≤60 Quenching and Tempering 600~750 ≥350 ≥19 ≥45 ≥20
d≤16;t≤16 Normalizing (N) ≥580 ≥320 ≥16
16<d≤100;16<t≤100 Normalizing (N) ≥550 ≥290 ≥17
100<d≤250;100<t≤250 Normalizing (N) ≥530 ≥260 ≥17
New and Old Grade Replacement List
Corresponding Standard Grade
DIN 17200-1987
Grade
Germany W-Nr.
DIN EN ISO 683-1-2018
Grade
C40R Corresponding Standards(Same grade name, different standards)