Grade C45R
Corresponding Standard DIN EN ISO 683-1-2018
Heat-treatable steels,alloy steels and free-cutting steels--Part 1: Non-alloy steels for quenching and tempering
Classification Carbon Steel
C45R Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.42 0.1 0.5 - 0.02 - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.5 0.4 0.8 0.025 0.04 0.4 0.4 0.3 0.1
C45R Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
d≤16; t≤8 Quenching and Tempering 700~850 ≥490 ≥14 ≥35 ≥15
16<d≤40;8<t≤20 Quenching and Tempering 650~800 ≥430 ≥16 ≥40 ≥15
40<d≤100;20<t≤60 Quenching and Tempering 630~780 ≥370 ≥17 ≥45 ≥15
d≤16;t≤16 Normalizing (N) ≥620 ≥340 ≥14
16<d≤100;16<t≤100 Normalizing (N) ≥580 ≥305 ≥16
100<d≤250;100<t≤250 Normalizing (N) ≥560 ≥275 ≥16
All Sizes Shearable Condition (+S) ≤255
All Sizes Softening Annealing (+A) ≤207
d≤100;t≤100 Flame or Induction Quenching HRC
≥55
New and Old Grade Replacement List
Corresponding Standard Grade
DIN 17200-1987
Grade
Germany W-Nr.
DIN EN ISO 683-1-2018
Grade
C45R Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!