Grade C55R
Corresponding Standard DIN EN ISO 683-1-2018
Heat-treatable steels,alloy steels and free-cutting steels--Part 1: Non-alloy steels for quenching and tempering
Classification Carbon Steel
C55R Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.52 0.1 0.6 - 0.02 - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.6 0.4 0.9 0.025 0.04 0.4 0.4 0.3 0.1
C55R Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
d≤16; t≤8 Quenching and Tempering 800~950 ≥550 ≥12 ≥30
16<d≤40;8<t≤20 Quenching and Tempering 750~900 ≥490 ≥14 ≥35
40<d≤100;20<t≤60 Quenching and Tempering 700~850 ≥420 ≥15 ≥40
d≤16;t≤16 Normalizing (N) ≥680 ≥370 ≥11
16<d≤100;16<t≤100 Normalizing (N) ≥640 ≥330 ≥12
100<d≤250;100<t≤250 Normalizing (N) ≥620 ≥300 ≥12
All Sizes Shearable Condition (+S) ≤255
All Sizes Softening Annealing (+A) ≤229
d≤100;t≤100 Flame or Induction Quenching HRC
≥58
New and Old Grade Replacement List
Corresponding Standard Grade
DIN 17200-1987
Grade
Germany W-Nr.
DIN EN ISO 683-1-2018
Grade
C55R Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!