Grade C60
Corresponding Standard DIN EN ISO 683-1-2018
Heat-treatable steels,alloy steels and free-cutting steels--Part 1: Non-alloy steels for quenching and tempering
Classification Carbon Steel
C60 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.57 0.1 0.6 - - - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.65 0.4 0.9 0.045 0.045 0.4 0.4 0.3 0.1
C60 Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
d≤16; t≤8 Quenching and Tempering 850~1000 ≥580 ≥11 ≥25
16<d≤40;8<t≤20 Quenching and Tempering 800~950 ≥520 ≥13 ≥30
40<d≤100;20<t≤60 Quenching and Tempering 750~900 ≥450 ≥14 ≥35
d≤16;t≤16 Normalizing (N) ≥710 ≥380 ≥10
16<d≤100;16<t≤100 Normalizing (N) ≥670 ≥340 ≥11
100<d≤250;100<t≤250 Normalizing (N) ≥650 ≥310 ≥11
All Sizes Shearable Condition (+S) ≤255
New and Old Grade Replacement List
Corresponding Standard Grade
DIN 17200-1987
Grade
Germany W-Nr.
DIN EN ISO 683-1-2018
Grade
1 Approximate Comparison Table
China Japan United States International Organization for Standardization Germany European Standard Russia United Kingdom
GB JIS ASTM ISO DIN EN/DIN EN Numerical Grade GOST BS EN/BS
60 S58C 1060 C60 C60 C60 1.0601 60
60G
070M60
2 Approximate Comparison Table
China Japan United States International Organization for Standardization Germany France Russia United Kingdom
GB JIS ASTM/AISI ISO DIN EN/DIN W-Nr. NF EN/NF GOST BS EN/BS
60Mn SWRH62B 1060
1061
Type SC
Type DC
C60 1.0601 C60 60г C60
080A57
080A62

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!