Grade
X10CrNi 18-8
European Standard Steel Grade
1.4310
Corresponding Standard
EN 10088-3-2014
Stainless steels-Part 3: Technical delivery condition for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes
Classification
Austenitic Stainless Steel
Properties
Corrosion Resistance
Density
7.9 g/cm3
X10CrNi 18-8 Chemical Element Composition Content (%)
Component
C
Si
Mn
P
S
Cr
Ni
Mo
N
Minimum Value
0.05
-
-
-
-
16
6
-
-
Maximum Value
0.15
2
2
0.045
0.015
19
9.5
0.8
0.1
X10CrNi 18-8 Mechanical Properties
condition
Heat Treatment or Condition
Tensile Strength σb
Mpa
Yield Point σs
Mpa
Elongation or Extension Rate δ
%
Hardness
HBW
Bars, rods, wire rods, profiles, bright products; d≤40
+AT
500~750
≥195
≥40
≤230
Bar;
+C800
800~1000
≥500
≥12
-
Cold drawn wire; d≥0.05
+C500
500~700
Cold drawn wire; d≥0.05
+C600
600~800
Cold drawn wire; d≥0.05
+C700
700~900
Cold drawn wire; d≥0.05
+C800
800~1000
Cold drawn wire; d≥0.05
+C900
900~1100
Cold drawn wire; d≥0.05
+C1000
1000~1250
Cold drawn wire; d≥0.05
+C1100
1100~1350
Cold drawn wire; d≥0.05
+C1200
1200~1450
Cold drawn wire; d≥0.05
+C1400
1400~1700
Cold drawn wire; d≥0.05
+C1600
1600~1900
Cold drawn wire; d≥0.05
+C1800
1800~2100
Cold drawn wire; 0.05<d≤0.1
+AT
≤1100
≥20
Cold drawn wire; 0.1<d≤0.2
+AT
≤1050
≥20
Cold drawn wire; 0.2<d≤0.5
+AT
≤1000
≥30
Cold drawn wire; 0.5<d≤1
+AT
≤950
≥30
Cold drawn wire; 1<d≤3
+AT
≤900
≥30
Cold drawn wire; 3<d≤5
+AT
≤850
≥35
Cold-drawn wire; 5<d≤16
+AT
≤800
≥35
1 Approximate Comparison Table
2 Approximate Comparison Table
3 Approximate Comparison Table
4 Approximate Comparison Table Stainless steels for cold heading and cold extruding