Grade X3CrNiCu18-9-4
European Standard Steel Grade 1.4567
Corresponding Standard EN 10088-3-2014
Stainless steels-Part 3: Technical delivery condition for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
X3CrNiCu18-9-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu N
Minimum Value - - - - - 17 8.5 3 -
Maximum Value 0.04 1 2 0.045 0.03 19 10.5 4 0.1
X3CrNiCu18-9-4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Bar, rod, wire, section, bright products; d≤160 +AT 450~650 ≥175 ≥45 ≤215
Cold drawn, precision bar; d≤10 +AT 600~850 ≥25
Cold drawn, precision bar; 10<d≤16 +AT 600~850 ≥25
Cold drawn, precision bar; 16<d≤40 +AT 450~800 ≥30 ≥100
Cold drawn, precision bar; 40<d≤63 +AT 450~800 ≥30 ≥100
Cold drawn, precision bar; 63<d≤160 +AT 450~650 ≥40 ≥100
Cold drawn wire; d≥0.05 +C500 500~700
Cold drawn wire; d≥0.05 +C600 600~800
Cold drawn wire; d≥0.05 +C700 700~900
Cold drawn wire; d≥0.05 +C800 800~1000
Cold drawn wire; d≥0.05 +C900 900~1100
Cold drawn wire; d≥0.05 +C1000 1000~1250
Cold drawn wire; d≥0.05 +C1100 1100~1350
Cold drawn wire; d≥0.05 +C1200 1200~1450
Cold drawn wire; d≥0.05 +C1400 1400~1700
Cold drawn wire; d≥0.05 +C1600 1600~1900
Cold drawn wire; d≥0.05 +C1800 1800~2100
Cold drawn wire; 0.05<d≤0.1 +AT ≤1100 ≥20
Cold drawn wire; 0.1<d≤0.2 +AT ≤1050 ≥20
Cold drawn wire; 0.2<d≤0.5 +AT ≤1000 ≥30
Cold drawn wire; 0.5<d≤1 +AT ≤950 ≥30
Cold drawn wire; 1<d≤3 +AT ≤900 ≥30
Cold drawn wire; 3<d≤5 +AT ≤850 ≥35
Cold-drawn wire; 5<d≤16 +AT ≤800 ≥35
1 Approximate Comparison Table Austenitic Stainless Steel
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard
GB ISC CNS JIS KS ASTM/AISI UNS ISO Numerical Grade DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade
06Cr18Ni9Cu3 S30488 XM7 SUS XM7 STS XM7 XM7 S30430 X3CrNiCu 18-9-4 4567-304-30-I X3CrNiCu 18-9 1.4567 Z3CNU 18-10 X3CrNiCu 18-9-4 1.4567
2 Approximate Comparison Table Austenitic Stainless Steel
China Japan International Organization for Standardization European Standard
ISC JIS ISO Numerical Grade Numerical Grade
S30480 SUS304J1 X6CrNiCu17-8-2 4567-304-76-I 1.4567
3 Approximate Comparison Table Austenitic Stainless Steel
China Japan International Organization for Standardization European Standard
ISC JIS ISO Numerical Grade Numerical Grade
S30480 SUS304J3 X6CrNiCu18-9-2 4567-304-98-X 1.4567
4 Approximate Comparison Table Austenitic Stainless Steel
Japan United States France European Standard United Kingdom
JIS UNS NF EN/NF EN Numerical Grade BS EN/BS
SUSXM7 S30430 Z3CNU18-09FF
Z3CNU18-10
Z3CNU18-10FF
X3CrNiCu18-9-4 1.4567 304S17
5 Approximate Comparison Table Stainless Steels for Cold Heading and Cold Extruding
China Japan International Organization for Standardization European Standard
GB ISC JIS ISO Numerical Grade EN Numerical Grade
06Cr18Ni9Cu2
(0Cr18Ni9Cu2)
S30480 SUS304J3 X6CrNiCu18-9-2 4567-304-98-X X6CrNiCu18-9-2 1.4567
6 Approximate Comparison Table Stainless Steels for Cold Heading and Cold Extruding
China Japan International Organization for Standardization European Standard
GB ISC JIS ISO Numerical Grade EN Numerical Grade
06Cr18Ni9Cu3
(0Cr18Ni9Cu3)
S30488 SUSXM7 X3CrNiCu18-9-4 4567-304-30-I X3CrNiCu18-9-4 1.4567

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!