Grade X2CrNiMoN 17-11-2
European Standard Steel Grade 1.4406
Corresponding Standard EN 10088-3-2014
Stainless Steels-Part 3: Technical Delivery Conditions for Semi-Finished Products, Bars, Rods, Wire, Sections and Bright Products of Corrosion Resisting Steels for General Purposes
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
X2CrNiMoN 17-11-2 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N
Minimum Value - - - - - 16.5 10 2 0.12
Maximum Value 0.03 1 2 0.045 0.03 18.5 12.5 2.5 0.22
X2CrNiMoN 17-11-2 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Bar, rod, wire, section, bright products; d≤160 +AT 580~800 ≥280 (long.)
≥40
≤250 (long.)
≥100
Bar, rod, wire, section, bright products; 160<d≤250 +AT 580~800 ≥280 (tr.)
≥30
≤250 (tr.)
≥60
Approximate Comparison Table Austenitic Stainless Steel
Japan United States France European Standard United Kingdom
JIS ASTM NF EN/NF EN Numerical Grade BS EN/BS
SUS316LN 316LN Z3CND17-11Az X2CrNiMoN17-11-2 1.4406 316S61

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!