Grade X5CrNi 17-7
European Standard Steel Grade 1.4319
Corresponding Standard EN 10088-3-2014
Stainless steels-Part 3: Technical Delivery Condition for Semi-Finished Products, Bars, Rods, Wire, Sections and Bright Products of Corrosion Resisting Steels for General Purposes
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
Density 7.9 g/cm3
X5CrNi 17-7 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni N
Minimum Value - - - - - 16 6 -
Maximum Value 0.07 1 2 0.045 0.03 18 8 0.1
X5CrNi 17-7 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Bar, Rod, Wire, Section, Bright Products; d≤16 +AT 500~700 ≥190 (long.)
≥45
≤215 (long.)
≥100

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!