Grade X11CrNiMnN 19-8-6
European Standard Steel Grade 1.4369
Corresponding Standard EN 10088-3-2014
Stainless steels-Part 3: Technical delivery condition for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
Density 7.9 g/cm3
X11CrNiMnN 19-8-6 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni N
Minimum Value 0.07 0.5 5 - - 17.5 6.5 0.2
Maximum Value 0.15 1 7.5 0.03 0.015 19.5 8.5 0.3
X11CrNiMnN 19-8-6 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Bar stock, rod stock, wire, profiles, bright products; d ≤ 15 +AT 750~950 ≥340 (long.)
≥35
≤300 (long.)
≥100
Bar stock, rod stock, wire, profiles, bright products; d ≤ 15 +AT 750~950 ≥340 (tr.)
≥35
≤300 (tr.)
≥60
Approximate Comparison Table
International Organization for Standardization European Standard
ISO Numerical Grade Numerical Grade
X11CrNiMnN19-8-6 4369-202-91-I 1.4369