Grade
X7CrNiAl 17-7
European Standard Steel Grade
1.4568
Corresponding Standard
EN 10088-3-2014
Stainless steels-Part 3: Technical delivery condition for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes
Classification
Precipitation-Hardening Stainless Steel
Properties
Corrosion Resistance
Density
7.8 g/cm3
X7CrNiAl 17-7 Chemical Element Composition Content (%)
Component
C
Si
Mn
P
S
Cr
Ni ⓓ
Al
Minimum Value
-
-
-
-
-
16
6.5
0.7
Maximum Value
0.09
0.7
1
0.04
0.015
18
7.8
1.5
X7CrNiAl 17-7 Mechanical Properties
condition
Heat Treatment or Condition
Tensile Strength σb
Mpa
Elongation or Extension Rate δ
%
Reduction of Area ψ
%
Bar, Rod, Wire, Profile, Bright Products; d≤30
+AT
≤850
≤255
Cold drawn wire; d≥0.05
+C500
500~700
Cold drawn wire; d≥0.05
+C600
600~800
Cold drawn wire; d≥0.05
+C700
700~900
Cold drawn wire; d≥0.05
+C800
800~1000
Cold drawn wire; d≥0.05
+C900
900~1100
Cold drawn wire; d≥0.05
+C1000
1000~1250
Cold drawn wire; d≥0.05
+C1100
1100~1350
Cold drawn wire; d≥0.05
+C1200
1200~1450
Cold drawn wire; d≥0.05
+C1400
1400~1700
Cold drawn wire; d≥0.05
+C1600
1600~1900
Cold drawn wire; d≥0.05
+C1800
1800~2100
Cold drawn wire; 0.5<d≤1
+AT
≤1100
≥10
Cold drawn wire; 1<d≤3
+AT
≤1050
≥10
Cold drawn wire; 3<d≤5
+AT
≤1000
≥10
Cold-drawn wire; 5<d≤16
+AT
≤950
≥15
1 Approximate Comparison Table Precipitation Hardening Stainless Steel
2 Approximate Comparison Table Precipitation Hardening Heat-Resistant Steel
3 Approximate Comparison Table Precipitation Hardening Stainless Steel
X7CrNiAl17-7 Corresponding Standards(Same grade name, different standards)
Message