Grade X2CrTi 17
Germany W-Nr. 1.4520
Corresponding Standard DIN EN 10088-3-2014
Stainless steels – Part 3: Technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes
Classification Ferritic Stainless Steel
Properties Corrosion Resistance
Density 7.7 g/cm3
X2CrTi 17 Chemical Element Composition Content (%)
Component C Si Mn P S Cr N More
Minimum Value - - - - - 16 - Ti:[4x(C+N) + 0.15] ~0.80*
Maximum Value 0.025 0.5 0.5 0.04 0.015 18 0.015
① Elements not quoted in this table shall not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast. All precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production which would impair mechanical properties and the suitability of the steel.
X2CrTi 17 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Bar, rod, wire, section, bright products; d≤50 +A 420~620 ≥200 ≥20 ≤200
Cold drawn, precision bar; d≤10 +A 500~750 ≥320 ≥8
Cold drawn, precision bar; 10<d≤16 +A 480~750 ≥300 ≥10
Cold drawn, precision bar; 16<d≤40 +A 400~700 ≥240 ≥15
Cold Drawn, Precision Finished Bar; 40<d≤50 +A 400~700 ≥240 ≥15
+AT=solution annealed;+A=annealed;+QT = quenched and tempered;+P=precipitation hardening;+C=Cold worked,+Csuffix followed by a number represents the tensile strength grade, i.e., the minimum tensile strength value.
long.=longitudinal;tr.=transverse
d=diameter or thickness;Unit mm

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!