Grade X3CrNb 17
European Standard Steel Grade 1.4511
Corresponding Standard EN 10088-3-2014
Stainless steels-Part 3: Technical delivery condition for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes
Classification Ferritic Stainless Steel
Properties Corrosion Resistance
Density 7.7 g/cm3
X3CrNb 17 Chemical Element Composition Content (%)
Component C Si Mn P S Cr More
Minimum Value - - - - - 16 Nb: 12xC~1
Maximum Value 0.05 1 1 0.04 0.03 18
X3CrNb 17 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Bar, rod, wire, section, bright products; d≤50 +A 420~620 ≥200 ≥20 ≤200
Cold drawn, precision bar; d≤10 +A 500~750 ≥320 ≥8
Cold drawn, precision bar; 10<d≤16 +A 480~750 ≥300 ≥10
Cold drawn, precision bar; 16<d≤40 +A 400~700 ≥240 ≥15
Cold Drawn, Precision Finished Bar; 40<d≤50 +A 400~700 ≥240 ≥15
Cold drawn wire; d≥0.05 +C500 500~700
Cold drawn wire; d≥0.05 +C600 600~800
Cold drawn wire; d≥0.05 +C700 700~900
Cold drawn wire; d≥0.05 +C800 800~1000
Cold drawn wire; d≥0.05 +C900 900~1100
Cold drawn wire; 0.05<d≤0.1 +A ≤950 ≥10
Cold drawn wire; 0.1<d≤0.2 +A ≤900 ≥10
Cold drawn wire; 0.2<d≤0.5 +A ≤850 ≥15
Cold drawn wire; 0.5<d≤1 +A ≤850 ≥15
Cold drawn wire; 1<d≤3 +A ≤800 ≥15
Cold drawn wire; 3<d≤5 +A ≤750 ≥15
Cold-drawn wire; 5<d≤16 +A ≤700 ≥20
Approximate Comparison Table Ferritic Stainless Steel
Japan International Organization for Standardization European Standard
JIS ISO Numerical Grade Numerical Grade
SUS430LX X3CrNb17 4511-430-71-I 1.4511

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!