Grade CuNi12Zn24
European Standard Steel Grade CW403J
Corresponding Standard EN 12166-2016
Copper and copper alloys - Wire for general purposes
Classification Copper and Copper Alloys
Density 8.7 g/cm3
CuNi12Zn24 Chemical Element Composition Content (%)
Component Fe Mn Ni Cu Pb Sn Other Total More
Minimum Value - - 11 63 - - - Zn:余量
Maximum Value 0.3 0.5 13 66 0.03 0.03 0.2
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
CuNi12Zn24 Mechanical Properties
diameter*
d
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
1.5<d≤20 CuNi12Zn24-H090 H090 HV
90~130
1.5<d≤12 CuNi12Zn24-H130 H130 130~160
1.5<d≤10 CuNi12Zn24-H170 H170 170~200
1.5<d≤4 CuNi12Zn24-H200 H200 ≥200
d≤1.5 CuNi12Zn24-H220 H220 ≥220
1.5<d≤20 CuNi12Zn24-R380 R380 ≥380 ≤290 ≥28(A100),
≥33(A11.3)
≥38(A)
1.5<d≤12 CuNi12Zn24-R450 R450 ≥450 ≥200 ≥8(A100),
≥10(A11.3),
≥12(A)
0.1<d≤10 CuNi12Zn24-R540 R540 ≥540 ≥400 ≥2(A100),
≥3(A11.3),
≥5(A)
0.1<d≤4 CuNi12Zn24-R640 R640 ≥640 ≥500
0.1<d≤1.5 CuNi12Zn24-R800 R800 ≥800 ≥700
All specifications CuNi12Zn24-M M No specification No specification No specification No specification
Approximate Comparison Table Cupper and cupper alloy
Germany European Standard
DIN EN/DIN W-Nr. EN Numerical Grade
CuNi12Zn24 2.0730 CuNi12Zn24 CW403J

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!