Grade 11SMnPb30
Corresponding Standard DIN EN ISO 683-4-2018
Heat-treatable steels,alloy steels and free-cutting steels--Part 4: free-cutting steels
Classification Carbon Steel
Properties Machinability
11SMnPb30 Chemical Element Composition Content (%)
Component C Si Mn P S Pb
Minimum Value - - 0.9 - 0.27 0.2
Maximum Value 0.14 0.05 1.3 0.11 0.33 0.35
11SMnPb30 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Hardness
HBW
5<d≤40 Untreated (U) 380~570 ≤169
40<d≤63 Untreated (U) 370~570 ≤169
63<d≤100 Untreated (U) 360~520 ≤154
New and Old Grade Replacement List
Corresponding Standard Grade
DIN 1651-1988
Grade
Germany W-Nr.
DIN EN ISO 683-4-2018
Grade

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!