Grade 36SMnPb14
Corresponding Standard DIN EN ISO 683-4-2018
Heat-treatable steels,alloy steels and free-cutting steels--Part 4: free-cutting steels
Classification Alloy Steel
Properties Machinability Quench Hardness
36SMnPb14 Chemical Element Composition Content (%)
Component C Si Mn P S Pb
Minimum Value 0.32 - 1.3 - 0.1 0.15
Maximum Value 0.39 0.4 1.7 0.06 0.18 0.35
36SMnPb14 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
5<d≤10 Untreated (U) 580~770 ≤225
10<d≤16 Untreated (U) 580~770 ≤225
16<d≤40 Untreated (U) 560~750 ≤219
40<d≤63 Untreated (U) 560~740 ≤216
63<d≤100 Untreated (U) 550~740 ≤216
5<d≤10 Quenching and Tempering 700~850 ≥480 ≥14
10<d≤16 Quenching and Tempering 700~850 ≥460 ≥14
16<d≤40 Quenching and Tempering 670~820 ≥420 ≥15
40<d≤63 Quenching and Tempering 640~790 ≥400 ≥16
63<d≤100 Quenching and Tempering 570~720 ≥360 ≥17

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!