Grade 11SMn30
Corresponding Standard ISO 683-4-2016
Heat-Treatable Steels,Alloy Steels and Free-Cutting Steels--Part 4: Free-Cutting Steels
Classification Carbon Steel
Properties Machinability
11SMn30 Chemical Element Composition Content (%)
Component C Si Mn P S
Minimum Value - - 0.9 - 0.27
Maximum Value 0.14 0.05 1.3 0.11 0.33
①Elements not quoted shall not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast. All reasonable precautions are to be taken to avoid the addition of such elements from scrap and other materials used in manufacture which affect the mechanical properties and the suitability. However, if agreed, the manufacturer can add elements such as Ca, Se,Te, etc. for the purpose of improving the machinability. These elements have to be reported in the inspection document.
11SMn30 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Hardness
HBW
5<d≤40 Untreated (U) 380~570 ≤169
40<d≤63 Untreated (U) 370~570 ≤169
63<d≤100 Untreated (U) 360~520 ≤154
Approximate Comparison Table Free-Cutting Structural Steel
China Japan United States International Organization for Standardization Germany France European Standard
GB JIS SAE ISO DIN EN/DIN NF EN/NF EN Numerical Grade
Y15 SUM22 1215 11SMn30 9SMn28 S250 11SMn30 1.0715

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!