Grade C25R
Corresponding Standard ISO 683-18-2014
Heat-treatable Steels, Alloy Steels and Free-Cutting Steels - Part 18: Bright Steel Products
Classification Carbon Steel
C25R Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.22 0.1 0.4 - 0.02 - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.29 0.4 0.7 0.025 0.04 0.4 0.4 0.3 0.1
C25R Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
5≤t≤10 Cold drawn (+C) 560~860 ≥420 ≥6
10<t≤16 Cold drawn (+C) 530~880 ≥380 ≥7
16<t≤40 Cold drawn (+C) 510~810 ≥300 ≥8
40<t≤63 Cold drawn (+C) 490~790 ≥265 ≥9
63<t≤100 Cold drawn (+C) 440~740 ≥245 ≥10
16<t≤100 As-rolled + peeled (+SH) 440~640 130~187
16<t≤40 Quenched and tempered and peeled (+QT+SH) 500~650 ≥320 ≥20 ≥45
Approximate Comparison Table Non-Alloy Steel for Quenching and Tempering
International Organization for Standardization Germany France European Standard
ISO DIN EN/DIN NF EN/NF EN Numerical Grade
C25R Cm22 XC18u C22R
C22R
1.1149
C25R Corresponding Standards(Same grade name, different standards)