Grade C50E
Corresponding Standard ISO 683-18-2014
Heat-treatable Steels, Alloy Steels and Free-Cutting Steels - Part 18: Bright Steel Products
Classification Carbon Steel
C50E Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.47 0.1 0.6 - - - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.55 0.4 0.9 0.025 0.035 0.4 0.4 0.3 0.1
C50E Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
5≤t≤10 Cold drawn (+C) 770~1100 ≥590 ≥5
10<t≤16 Cold drawn (+C) 730~1080 ≥520 ≥6
16<t≤40 Cold drawn (+C) 690~1050 ≥440 ≥7
40<t≤63 Cold drawn (+C) 650~1030 ≥390 ≥8
16<t≤100 As-rolled + peeled (+SH) 610~910 179~269
16<t≤40 Quenched and tempered and peeled (+QT+SH) 700~850 ≥460 ≥15
40<t≤100 Quenched and tempered and peeled (+QT+SH) 650~800 ≥400 ≥16
5≤t≤10 Quenched and tempered + cold drawn (+QT +C) 870~1070 ≥610 ≥7
10<t≤16 Quenched and tempered + cold drawn (+QT +C) 830~1030 ≥580 ≥7
16<t≤40 Quenched and tempered + cold drawn (+QT +C) 790~990 ≥555 ≥8
40<t≤63 Quenched and tempered + cold drawn (+QT +C) 730~930 ≥510 ≥9
63<t≤100 Quenched and tempered + cold drawn (+QT +C) 680~880 ≥475 ≥9
Approximate Comparison Table Non-Alloy Steel for Quenching and Tempering
China Japan International Organization for Standardization European Standard
GB JIS ISO EN Numerical Grade
50 S50C C50E C50E 1.1206
C50E Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!