Grade C50R
Corresponding Standard ISO 683-18-2014
Heat-treatable Steels, Alloy Steels and Free-Cutting Steels - Part 18: Bright Steel Products
Classification Carbon Steel
C50R Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo More
Minimum Value 0.47 0.1 0.6 - 0.02 - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.55 0.4 0.9 0.025 0.04 0.4 0.4 0.3 0.1
C50R Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
5≤t≤10 Cold drawn (+C) 770~1100 ≥590 ≥5
10<t≤16 Cold drawn (+C) 730~1080 ≥520 ≥6
16<t≤40 Cold drawn (+C) 690~1050 ≥440 ≥7
40<t≤63 Cold drawn (+C) 650~1030 ≥390 ≥8
16<t≤100 As-rolled + peeled (+SH) 610~910 179~269
16<t≤40 Quenched and tempered and peeled (+QT+SH) 700~850 ≥460 ≥15
40<t≤100 Quenched and tempered and peeled (+QT+SH) 650~800 ≥400 ≥16
5≤t≤10 Quenched and tempered + cold drawn (+QT +C) 870~1070 ≥610 ≥7
10<t≤16 Quenched and tempered + cold drawn (+QT +C) 830~1030 ≥580 ≥7
16<t≤40 Quenched and tempered + cold drawn (+QT +C) 790~990 ≥555 ≥8
40<t≤63 Quenched and tempered + cold drawn (+QT +C) 730~930 ≥510 ≥9
63<t≤100 Quenched and tempered + cold drawn (+QT +C) 680~880 ≥475 ≥9
Approximate Comparison Table Non-Alloy Steel for Quenching and Tempering
United States International Organization for Standardization Germany European Standard
ASTM ISO DIN EN/DIN EN Numerical Grade
1050 C50R
C50M2
Cm50 C50R 1.1241
C50R Corresponding Standards(Same grade name, different standards)