Grade 25CrMoS4
Corresponding Standard ISO 683-18-2014
Heat-treatable Steels, Alloy Steels and Free-Cutting Steels - Part 18: Bright Steel Products
Classification Alloy Steel
25CrMoS4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Cu Mo
Minimum Value 0.22 0.1 0.6 - 0.02 0.9 - 0.15
Maximum Value 0.29 0.4 0.9 0.025 0.04 1.2 0.4 0.3
25CrMoS4 Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
16<t≤100 S.annealed +peeled (+A +SH) ≤212
5≤t≤10 S.annealed +Cold drawn (+A +C) ≤270
10<t≤16 S.annealed +Cold drawn (+A +C) ≤260
16<t≤40 S.annealed +Cold drawn (+A +C) ≤255
40<t≤100 S.annealed +Cold drawn (+A +C) ≤250
16<t≤40 Quenched and tempered and peeled (+QT+SH) 800~950 ≥600 ≥14 ≥50
40<t≤100 Quenched and tempered and peeled (+QT+SH) 700~850 ≥450 ≥15 ≥50
5≤t≤16 Quenched and tempered + Cold drawn (+QT +C) 900~1100 ≥700 ≥9
16<t≤40 Quenched and tempered + Cold drawn (+QT +C) 800~1000 ≥600 ≥10
40<t≤63 Quenched and tempered + Cold drawn (+QT +C) 700~900 ≥520 ≥11
63<t≤100 Quenched and tempered + Cold drawn (+QT +C) 700~900 ≥450 ≥12
1 Approximate Comparison Table Alloy Steel for Quenching and Tempering
International Organization for Standardization Germany France European Standard
ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade
25CrMoS4 25CrMoS4 1.7213 25CD4u 25CrMoS4 1.7213
2 Approximate Comparison Table Steel for Cold Heading and Cold Extrusion
International Organization for Standardization European Standard
ISO EN Numerical Grade
25CrMoS4 25CrMoS4 1.7213

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!