Grade 34CrNiMo6
Corresponding Standard ISO 683-18-2014
Heat-treatable Steels, Alloy Steels and Free-Cutting Steels - Part 18: Bright Steel Products
Classification Alloy Steel
34CrNiMo6 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo
Minimum Value 0.3 0.1 0.5 - - 1.3 1.3 - 0.15
Maximum Value 0.38 0.4 0.8 0.025 0.035 1.7 1.7 0.4 0.3
34CrNiMo6 Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
16<t≤100 S.annealed +peeled (+A +SH) ≤248
5≤t≤10 S.annealed +Cold drawn (+A +C) ≤308
10<t≤16 S.annealed +Cold drawn (+A +C) ≤298
16<t≤40 S.annealed +Cold drawn (+A +C) ≤293
40<t≤100 S.annealed +Cold drawn (+A +C) ≤288
16<t≤40 Quenched and tempered and peeled (+QT+SH) 1100~1300 ≥900 ≥10 ≥40
40<t≤100 Quenched and tempered and peeled (+QT+SH) 1000~1200 ≥800 ≥11 ≥45
5≤t≤10 Quenched and tempered + Cold drawn (+QT +C) 1000~1200 ≥770 ≥8
10<t≤16 Quenched and tempered + Cold drawn (+QT +C) 1000~1200 ≥750 ≥8
16<t≤40 Quenched and tempered + Cold drawn (+QT +C) 1000~1200 ≥720 ≥9
40<t≤100 Quenched and tempered + Cold drawn (+QT +C) 1000~1200 ≥650 ≥10
1 Approximate Comparison Table Structural Alloy Steel
China International Organization for Standardization European Standard
GB ISO EN Numerical Grade
34Cr2Ni2Mo 34CrNiMo6 34CrNiMo6 1.6582
2 Approximate Comparison Table Steel for Cold Heading and Cold Extrusion
International Organization for Standardization European Standard
ISO EN Numerical Grade
34CrNiMo6 34CrNiMo6 1.6582

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!