Grade 25CrMoS4
Corresponding Standard EN ISO 683-2-2018
Heat-treatable steels,alloy steels and free-cutting steels--Part 2:Alloy steels for quenching and tempering
Classification Alloy Steel
25CrMoS4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Cu Mo
Minimum Value 0.22 0.1 0.6 - 0.02 0.9 - 0.15
Maximum Value 0.29 0.4 0.9 0.025 0.04 1.2 0.4 0.3
25CrMoS4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Bar, flat material, forging; d≤16 or t≤8 Quenching and Tempering (+QT) 900~1100 ≥700 ≥12 ≥50 - -
Bar, flat material, forging; 16<d≤40 or 8<t≤20 Quenching and Tempering (+QT) 800~950 ≥600 ≥14 ≥55 - ≥50
Bar, flat material, forging; 40<d≤100 or 20<t≤60 Quenching and Tempering (+QT) 700~850 ≥450 ≥15 ≥60 - ≥50
Bars, flat products, forgings; 100<d≤160 or 60<t≤100 Quenching and Tempering (+QT) 650~800 ≥400 ≥16 ≥60 - ≥45
Bars, semi-finished products Processed to improve shearability (+S) - - - - ≤255 -
Bars, flat products, forgings, semi-finished products, rebar Soft Annealing (+A) - - - - ≤212 -
1 Approximate Comparison Table
International Organization for Standardization Germany France European Standard
ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade
25CrMoS4 25CrMoS4 1.7213 25CD4u 25CrMoS4 1.7213
2 Approximate Comparison Table
International Organization for Standardization European Standard
ISO EN Numerical Grade
25CrMoS4 25CrMoS4 1.7213