Grade 34CrMoS4
Corresponding Standard EN ISO 683-2-2018
Heat-treatable steels,alloy steels and free-cutting steels--Part 2:Alloy steels for quenching and tempering
Classification Alloy Steel
34CrMoS4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Cu Mo
Minimum Value 0.3 0.1 0.6 - 0.02 0.9 - 0.15
Maximum Value 0.37 0.4 0.9 0.025 0.04 1.2 0.4 0.3
34CrMoS4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Bar, flat material, forging; d≤16 or t≤8 Quenching and Tempering (+QT) 1000~1200 ≥800 ≥11 ≥45 - -
Bar, flat material, forging; 16<d≤40 or 8<t≤20 Quenching and Tempering (+QT) 900~1100 ≥650 ≥12 ≥50 - ≥40
Bar, flat material, forging; 40<d≤100 or 20<t≤60 Quenching and Tempering (+QT) 800~950 ≥550 ≥14 ≥55 ≥45
Bars, flat products, forgings; 100<d≤160 or 60<t≤100 Quenching and Tempering (+QT) 750~900 ≥500 ≥15 ≥55 - ≥45
Bars, Flats, Forgings; 160<d≤250 or 100<t≤160 Quenching and Tempering (+QT) 700~850 ≥450 ≥15 ≥60 - ≥45
Bars, semi-finished products Processed to improve shearability (+S) - - - - ≤255 -
Bars, flat products, forgings, semi-finished products, rebar Soft Annealing (+A) - - - - ≤223 -
Approximate Comparison Table Alloy Steel for Quenching and Tempering
United States International Organization for Standardization Germany France European Standard
ASTM ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade
4135 34CrMoS4 34CrMoS4 1.7226 34CD4u 34CrMoS4 1.7226

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!