Grade 50CrMo4
Corresponding Standard EN ISO 683-2-2018
Heat-treatable steels,alloy steels and free-cutting steels--Part 2:Alloy steels for quenching and tempering
Classification Alloy Steel
Properties Machinability
50CrMo4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Cu Mo
Minimum Value 0.46 0.1 0.5 - - 0.9 - 0.15
Maximum Value 0.54 0.4 0.8 0.025 0.035 1.2 0.4 0.3
50CrMo4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Bar, flat material, forging; d≤16 or t≤8 Quenching and Tempering (+QT) 1100~1300 ≥900 ≥9 ≥40 - -
Bar, flat material, forging; 16<d≤40 or 8<t≤20 Quenching and Tempering (+QT) 1000~1200 ≥780 ≥10 ≥45 - ≥30
Bar, flat material, forging; 40<d≤100 or 20<t≤60 Quenching and Tempering (+QT) 900~1100 ≥700 ≥12 ≥50 - ≥30
Bars, flat products, forgings; 100<d≤160 or 60<t≤100 Quenching and Tempering (+QT) 850~1000 ≥650 ≥13 ≥50 - ≥30
Bars, Flats, Forgings; 160<d≤250 or 100<t≤160 Quenching and Tempering (+QT) 800~950 ≥550 ≥13 ≥50 - ≥30
Bars, flat products, forgings, semi-finished products, rebar Soft Annealing (+A) - - - - ≤248 -
1 Approximate Comparison Table
International Organization for Standardization European Standard
ISO EN Numerical Grade
50CrMo4 50CrMo4 1.7228
2 Approximate Comparison Table structural alloy steel
China Japan United States International Organization for Standardization Germany European Standard United Kingdom
GB JIS ASTM ISO W-Nr. L-Nr. EN Numerical Grade BS EN/BS
50CrMo SCM445 4150 50CrMo4 50CrMo4 1.7228 50CrMo4 1.7228 708M40
708M50