Grade X7CrNiAl17-7
Germany W-Nr. 1.4568
Corresponding Standard DIN EN 10270-3-2012
Steel Wire for Mechanical Springs – Part 3: Stainless Spring Steel Wire
Classification Precipitation-Hardening Stainless Steel
Properties Elasticity Corrosion Resistance
X7CrNiAl17-7 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni * Al
Minimum Value - - - - - 16 6.5 0.7
Maximum Value 0.09 0.7 1 0.04 0.015 18 7.8 1.5
X7CrNiAl17-7 Mechanical Properties
diameter
d
mm
Tensile Strength
σb
ksi
d ≤ 0.2 1975~2280
0.2 <d≤ 0.3 1950~2250
0.3<d≤ 0.4 1925~2220
0.4<d≤ 0.5 1900~2190
0.5<d≤ 0.65 1850~2130
0.65<d≤ 0.8 1825~2100
0.8<d≤ 1 1800~2070
1<d≤ 1.25 1750~2020
1.25<d≤ 1.5 1700~1960
1.5<d≤ 1.75 1650~1900
1.75<d≤ 2 1600~1840
2<d≤ 2.5 1550~1790
2.5<d≤ 3 1500~1730
3<d≤ 3.5 1450~1670
3.5<d≤ 4.25 1400~1610
4.25<d≤ 5 1350~1560
5<d≤ 6 1300~1500
6<d≤ 7 1250~1440
7<d≤ 8.5 1250~1440
8.5<d≤ 10 1240~1440
1 Approximate Comparison Table Precipitation Hardening Stainless Steel
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard Russia
GB ISC CNS JIS KS ASTM UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade GOST
07Cr17Ni7Al
(0Cr17Ni7Al)
S51770 631 SUS 631 STS 631 631 S17700 X7CrNiAl 17-7
2
(ISO 683-13-1986)
X7CrNiAl 17-7 1.4568 Z8CNA 17-07 X7CrNiAl 17-7 1.4568 09Х17Н7Ю
2 Approximate Comparison Table Precipitation Hardening Heat-Resistant Steel
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard Russia
GB ISC CNS JIS KS ASTM UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade GOST
07Cr17Ni7Al
(0Cr17Ni7Al)
S51770 631 SUS 631 STS 631 631 S17700 X7CrNiAl 17-7 X7CrNiAl 17-7 1.4568 Z8CNA 17-07 X7CrNiAl 17-7 1.4568 09Х17Н7Ю

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!