Grade 13CrMo 4-5
Corresponding Standard ISO 9328-2-2018
Steel flat products for pressure purposes - Non-alloy and alloy steels with specified elevated temperature properties
Classification Alloy Steel
13CrMo 4-5 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Cu Mo N
Minimum Value 0.08 - 0.4 - - 0.7 - 0.4 -
Maximum Value 0.18 0.35 1 0.025 0.01 1.15 0.3 0.6 0.012
13CrMo 4-5 Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤16 Normalizing and Tempering (+NT) 450~600 ≥300 ≥19 (+20℃)
≥31
16<t≤60 Normalizing and Tempering (+NT) 450~600 ≥290 ≥19 ≥31
60<t≤100 Normalizing and Tempering (+NT) 440~590 ≥270 ≥19 ≥27
100<t≤150 Normalizing and tempering or quenching and tempering (+NT or +QT) 430~580 ≥255 ≥19 ≥27
150<t≤250 Quenching and Tempering (+QT) 420~570 ≥245 ≥19 ≥27
Approximate Comparison Table
China United States International Organization for Standardization European Standard Russia
GB ASTM ISO EN Numerical Grade GOST
15CrMoR
GB/T 713.2-2023
SA387 Gr.12
ASME Ⅱ-A-2021
13CrMo4-5
ISO 9328-2018
13CrMo4-5
EN 10028-2017
1.7335 12ХМ

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!