Grade X10CrMoVNb 9-1
Corresponding Standard ISO 9328-2-2018
Steel flat products for pressure purposes - Non-alloy and alloy steels with specified elevated temperature properties
Classification Alloy Steel
X10CrMoVNb 9-1 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N V Nb Al
Minimum Value 0.08 - 0.3 - - 8 - - 0.85 0.03 0.18 0.06 -
Maximum Value 0.12 0.5 0.6 0.02 0.005 9.5 0.3 0.3 1.05 0.07 0.25 0.1 0.04
X10CrMoVNb 9-1 Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤60 Normalizing and Tempering (+NT) 580~760 ≥445 ≥18 (-20℃)
≥27
60<t≤150 Normalizing and Tempering (+NT) 550~730 ≥435 ≥18 ≥27
150<t≤250 Quenching and Tempering (+QT) 520~700 ≥435 ≥18 ≥27
Approximate Comparison Table Pressure-Bearing Flat Steel
International Organization for Standardization European Standard
ISO EN Numerical Grade
X10CrMoVNb 9-1 X10CrMoVNb 9-1 1.4903