Grade 34CrAlNi7-10
Corresponding Standard ISO 683-5-2017
Heat-Treatable Steels, Alloy Steels and Free-Cutting Steels — Part 5: Nitriding Steels
Classification Alloy Steel
34CrAlNi7-10 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo Al
Minimum Value 0.3 - 0.4 - - 1.5 0.85 0.15 0.8
Maximum Value 0.37 0.4 0.7 0.025 0.035 1.8 1.15 0.25 1.2
34CrAlNi7-10 Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
16≤d≤40, 8≤t≤20 Quenching and Tempering 900~1100 ≥680 ≥10 ≥30
40≤d≤100, 20≤t≤60 Quenching and Tempering 850~1050 ≥650 ≥12 ≥30
100≤d≤250, 60≤t≤160 Quenching and Tempering 800~1000 ≥600 ≥13 ≥35
Approximate Comparison Table Nitriding Steels
International Organization for Standardization European Standard
ISO EN Numerical Grade
34CrAlNi7-10 34CrAlNi7-10 1.8550
34CrAlNi7-10 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!