Grade 31CrMo12
Corresponding Standard ISO 683-5-2017
Heat-Treatable Steels, Alloy Steels and Free-Cutting Steels-- Part 5: Nitriding Steels
Classification Alloy Steel
31CrMo12 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo
Minimum Value 0.28 - 0.4 - - 2.8 - 0.3
Maximum Value 0.35 0.4 0.7 0.025 0.035 3.3 0.3 0.5
31CrMo12 Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
16≤d≤40, 8≤t≤20 Quenching and Tempering 1030~1230 ≥835 ≥10 ≥25
40≤d≤100, 20≤t≤60 Quenching and Tempering 980~1180 ≥785 ≥11 ≥30
100≤d≤160, 60≤t≤100 Quenching and Tempering 930~1130 ≥735 ≥12 ≥30
160≤d≤250, 100≤t≤160 Quenching and Tempering 880~1080 ≥675 ≥12 ≥30
Approximate Comparison Table Nitriding Steels
International Organization for Standardization Germany France European Standard United Kingdom
ISO DIN EN/DIN NF EN/NF EN Numerical Grade BS EN/BS
31CrMo12 31CrMo12 30CD12 31CrMo12 1.8515 722M24
31CrMo12 Corresponding Standards(Same grade name, different standards)