Grade CuNi30Mn1Fe
Germany W-Nr. CW354H
Corresponding Standard DIN EN 12163-2016
Copper and copper alloys – Rod for general purposes
Classification Copper and Copper Alloys
Density 8.9 g/cm3
CuNi30Mn1Fe Chemical Element Composition Content (%)
Component Fe C Mn P S Ni Co Pb Zn Sn Other Total More
Minimum Value 0.4 - 0.5 - - 30 - - - - - Cu:余量
Maximum Value 1 0.05 1.5 0.02 0.05 32 0.1 0.02 0.5 0.05 0.2
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
CuNi30Mn1Fe Mechanical Properties
diameter/width arcoss-flats
d/t
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
10<d/t≤80 CuNi30Mn1Fe-R340 R340 ≥340 ≥120 ≥30
10<d/t≤80 CuNi30Mn1Fe-H080 H080 80~110
2<d/t≤20 CuNi30Mn1Fe-R420 R420 ≥420 ≥180
2<d/t≤20 CuNi30Mn1Fe-H110 H110 ≥10(A100),
≥12(A11.3),
≥14(A)
≥110
All specifications CuNi30Mn1Fe-M M No specification No specification No specification No specification
①Material condition names and character codes:
H - Hardness (Brinell or Vickers hardness), with the suffix number indicating the hardness value.
R - Tensile strength, with the suffix number indicating the minimum tensile strength value.
M - Manufactured without specified mechanical properties.
Refer to standard EN 1173-2008.
②A100、A11.3、A-gauge length
New and Old Grade Replacement List
Approximate Comparison Table Copper and Copper Alloy
Germany European Standard
DIN EN/DIN W-Nr. EN Numerical Grade
CuNi30Mn1Fe 2.0882 CuNi30Mn1Fe CW354H

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!