Grade C85S
Germany W-Nr. 1.1269
Corresponding Standard DIN EN 10132-4-2000(+AC:2002)
Cold-Rolled Narrow Steel Strip for Heat Treatment-Technical Delivery Conditions Part 4: Spring Steels and Other Applications (Includes Corrigendum AC:2002)
Classification Spring Steel
C85S Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo
Minimum Value 0.8 0.15 0.4 - - - - -
Maximum Value 0.9 0.35 0.7 0.025 0.025 0.4 0.4 0.1
C85S Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
0.3≤t≤3 Annealing (+A) or Annealing and Flattening (+LC) ≤670 ≤535 ≥15 HV
≤210
0.3≤t≤3 Cold Rolled (+CR) ≤1190 ≤325
0.3≤t≤3 Tempering (+QT) 1200~2000 370~600
New and Old Grade Replacement List
Corresponding Standard Grade
DIN 17222-1979
Grade
Germany W-Nr.
DIN EN 10132-4-2000(+AC:2002)
Grade
Germany W-Nr.
Approximate Comparison Table Spring Steel
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard Russia Sweden United Kingdom
GB ISC CNS JIS KS AISI UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade GOST SS14 BS EN/BS
85 U20852 SUP3 SUP3 SPS1 1086 G10860 Type DC Ck85
C85S
1.1269
1.1269
XC85 C85S 1.1269 85A ≈1774 060A86