Grade Q355NC
Corresponding Standard GB /T 1591-2018
High Strength Low Alloy Structural Steels
Classification Alloy Steel
Q355NC Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N Ti V Nb Al
Minimum Value - - 0.9 - - - - - - - 0.006 0.01 0.005 0.015
Maximum Value 0.2 0.5 1.65 0.03 0.03 0.3 0.5 0.4 0.1 0.015 0.05 0.12 0.05 -
Q355NC Mechanical Properties
thickness or diameter
t
mm
Test Temperature Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤16 room temperature 470~630 ReH: ≥355 ≥22
16<t≤40 470~630 ReH: ≥345 ≥22
40<t≤63 470~630 ReH: ≥335 ≥22
63<t≤80 470~630 ReH: ≥325 ≥21
80<t≤100 470~630 ReH: ≥315 ≥21
100<t≤150 450~600 ReH: ≥295 ≥21
150<t≤200 450~600 ReH: ≥285 ≥21
200<t≤250 450~600 ReH: ≥275 ≥21
specimen 0°C long. ≥34
tr. ≥27
New and Old Grade Replacement List
Corresponding Standard Grade
GB /T 1591-1994
Grade
GB /T 1591-2008
Grade
China ISC
GB /T 1591-2018
Grade

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!