Grade TC4
Other Names
Corresponding Standard GB /T 3621-2007
Titanium and titanium alloy plate and sheet
Classification Titanium and Titanium Alloys
Density 4.44 g/cm3
TC4 Chemical Element Composition Content (%)
Component Fe C N V Al H O Other Individual Other Total More
Minimum Value - - - 3.5 5.5 - - - - Ti:余量
Maximum Value 0.3 0.08 0.05 4.5 6.75 0.015 0.2 0.1 0.4
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
TC4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hot-rolled, cold-rolled plate; 0.8≤t≤2 Annealed Condition (M) ≥895 ≥830 ≥12
Hot-rolled, cold-rolled sheet; 2 < t ≤ 5 Annealed Condition (M) ≥895 ≥830 ≥10
Hot-rolled, cold-rolled sheet; 5 < t ≤ 10 Annealed Condition (M) ≥895 ≥830 ≥10
Hot-rolled, Cold-rolled Plates; 10<t≤25 Annealed Condition (M) ≥895 ≥830 ≥8

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!