Grade X12CrNiTi18-9
1.4878
Corresponding Standard SEW 470(1976)
Heat-resisting rolled and forged steels
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
Density 7.9 g/cm3
X12CrNiTi18-9 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Ti
Minimum Value - - - - - 17 9 -
Maximum Value 0.12 1 2 0.045 0.03 19 12 0.8
X12CrNiTi18-9 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Steel plate, steel strip, steel pipe, steel bar, forged product, steel wire Normalizing 500~750 ≥210 40 ≤192

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!