Grade GH 4169
Corresponding Standard GJB 713-1989
GH 4169 Alloy rods for aerospace
Classification Nickel and Nickel Alloys
GH 4169 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo Ti Nb B * Co Al Mg More
Minimum Value - - - - - 17 50 - 2.8 0.65 4.75 - - 0.2 - Fe:余量
Maximum Value 0.08 0.35 0.35 0.015 0.015 21 55 0.3 3.3 1.15 5.5 0.006 1 0.8 0.01
GH 4169 Mechanical Properties
diameter
d
mm
Test Temperature Mark
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
16~115 Room Temperature Instantaneous Tensile Properties ≥1275 ≥1035 ≥12 ≥15 ≥331 ≥32
16~115 Instantaneous Tensile Properties ≥1000 ≥860 ≥12 ≥15 - -
16~115 Instantaneous Tensile Properties ≥1470 - ≥12 ≥20 - -
≥80 Room Temperature Instantaneous Tensile Properties ≥1275 ≥1030 ≥12 ≥15 ≥331 ≥39
≥80 Instantaneous Tensile Properties ≥540 - ≥15 ≥25 - -
≥80 Room Temperature Instantaneous Tensile Properties ≥1225 - ≥15 ≥30 341~477 ≥39
≥80 Instantaneous Tensile Properties ≥1080 - ≥12 ≥20 - -
<80 Room Temperature Instantaneous Tensile Properties ≥1225 - ≥15 ≥30 341~477 ≥39
<80 Instantaneous Tensile Properties ≥1130 - ≥12 ≥20 - -
<80 Instantaneous Tensile Properties ≥1470 - ≥12 ≥20 - -
16~115 Durability performance (690MPa) Life/h
≥25
≥4
≥80 Durability performance (390MPa) Life/h
≥30
≥80 Durability (880 MPa) Life/h
≥50
<80 Durability (880 MPa) Life/h
≥50
GH4169 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!