Grade GX10NiCrSiNb32-20
European Standard Steel Grade 1.4859
Corresponding Standard EN 10295-2002
Heat resistant steel castings
Classification Cast Steel
Density 8 g/cm3
GX10NiCrSiNb32-20 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu * Mo W * V * Nb Co *
Minimum Value 0.05 0.5 - - - 19 31 - - - - 0.5 -
Maximum Value 0.15 1.5 2 0.04 0.03 21 33 0.25 0.5 0.6 0.12 1.5 1
*The maximum content of the element is not specified
GX10NiCrSiNb32-20 Mechanical Properties
condition Test Temperature Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
cast steel Room Temperature ≥440 ≥180 ≥20
cast steel 700°C 100h (1000h) Rupture Strength σr 135(105) Creep Strength for 1%-10000h
64
cast steel 800°C 100h (1000h) Rupture Strength σr 84(60) Creep Strength for 1%-10000h
36
cast steel 900°C 100h (1000h) Rupture Strength σr 49(36) Creep Strength for 1%-10000h
15.5
cast steel 1000°C 100h (1000h) Rupture Strength σr 26(14) Creep Strength for 1%-10000h
5

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!