Grade G-CoCr28
European Standard Steel Grade 2.4778
Corresponding Standard EN 10295-2002
Heat resistant steel castings
Classification Cast Steel
Density 8.1 g/cm3
G-CoCr28 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu * Mo W * V * Nb Co More
Minimum Value 0.05 0.5 - - - 27 - - - - - - 48 Fe:余量
Maximum Value 0.25 1.5 1.5 0.04 0.03 30 4 0.25 0.5 0.6 0.12 0.5 52
*The maximum content of the element is not specified
G-CoCr28 Mechanical Properties
condition Test Temperature Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
cast steel Room Temperature ≥490 ≥235 ≥6
cast steel 700°C Creep
70
cast steel 800°C Creep
34
cast steel 900°C 100h (1000h) Rupture Strength σr 48(25) Creep
16
cast steel 1000°C 100h (1000h) Rupture Strength σr 23(12) Creep
9.5
cast steel 1100°C Creep
4
G-CoCr28 Corresponding Standards(Same grade name, different standards)