Grade 42SiMn
Corresponding Standard JB /T 6396-2006
Specification for the heavy alloy structural steel forings
Classification Alloy Steel
42SiMn Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu
Minimum Value 0.39 1.1 1.1 - - - - -
Maximum Value 0.45 1.4 1.4 0.035 0.035 0.3 0.3 0.2
42SiMn Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
≤100 Tempering ≥784 ≥509 ≥15 ≥45 235~286 ≥39
101~200 Tempering ≥735 ≥461 ≥14 ≥42 217~269 ≥29
201~300 Tempering ≥686 ≥441 ≥13 ≥40 207~255 ≥29
301~500 Tempering ≥637 ≥372 ≥10 ≥40 196~255 ≥25
42SiMn Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!